1.2365, SKD7, H10 Hot work tool steel

1)        Applications:
Highly stressed hot work tools in die forging presses for steels, brass and non ferrous metals, pressure casting dies for heavy and light metal alloys, mandrels, inner liners, stems, die holders, dummy blocks, pressure pads, bolsters, dies and containers for metal tube and rod extrusion, hot extrusion tools, single block inserts and dies for presses, tools for the manufacture of hollows, screws, nuts, bolts and rivets, hot shear blades, forging dies and press die inserts, die casting tools, hot forming dies, hot gripper and header dies.
 
2)        Chemical analysis:
C
Si
S
P
Mn
Cr
V
Mo
0.28~0.35
0.10~0.40
0.005
0.025
0.15~0.45
2.70~3.20
0.40~0.70
2.50~3.00
 
 
 
3)        Mechanical Properties:
 
Hot work tool steel with high resistance to thermal shocks and fatigue, good thermal conductivity, hot tensile and impact strength, resistance to tempering, fine grain size with high toughness, extra fine structure without grain boundary carbide, high creep strength at elevated temperature, insensitive to constant temperature change, low P and S content, suitable for water cooling. This grade can be produced on request by the process EFS, ESR or VAR.
 
4)        Condition of delivery:
 Soft annealed to max. 229 HB
 
5)        Compared grades, based on usage:
American
German
Japanese
EN
ASTM
DIN
JIS
ISO 4957
H10
1.2365
SKD7
32CrMoV12-28
 
6)        Available sizes:
   Round Bar: Φ 6-410mm
   Flat: 8-160*205-710mm
   Mould: 200*200-1200*1000mm
   Length: 3000-12000mm
Mill deliver conditions, or sawing or cutting for customer request.
 
7)       Physical properties:
 
Physical properties:
Temperature [oC]
20-100
20-250
20-500
20-600
Thermal expansion [10-6.K-1]
11.6
12.5
13.3
13.7
Temperature [oC]
20
350
700
 
Heat conductivity [W.m-1.K-1]
32.1
33.2
31.3
 
 
8)        Heattreatment:
>> Recommended temperatures for heat processing
 
 
Soft annealing:
Temperature [oC]
Cooling
 Hardness 
750-800
Furnace
 max. 229 HB 
Stress relief annealing
Temperature [oC]
Cooling
 
600-650
Furnace
  
Hardening:
Temperature  [oC]
Hardening
Tempering
1020-1050
Oil, pressure gas (N2), air or hot bath 500-550C
 see tempering
diagram
 

pressure vessels,boiler (BHW35,A537CL2,A299grB,A841grC,A387Gr11CL2,A516Gr70N+HIC,A515Gr60N,A203GrE,A517grQ), metallic structures(A36,A514GrB/P,S690QL,S890QL,S960Q,S355NL,S460NL,S355J2G3) offshore platform (EQ70,A709Gr100,A572Gr50,A514GrQ,API 2H50T,API 2W60,DNV DH36,EH36,FH36,EH40,FH40,E500). mould steel (S45C,P20,1.2311,1.2312,1.2738,NKA80,S136 ESR, 1.2316,1.2379,1.2344,1.2343,1.2803,1.2080,AISI M2) stainless steel, grades: 304, 304H, 304L, 316,316H,316L, 309S, 310S, 410,410S,17-4PH,2205,904L, 409L, 430,420,347,317L and so on.